Sample Young Modulus (MPa) Yield Strength (MPa) Ultimate Tensile Strength (MPa) Strain at Break (%)
C70 RG30(Manual) 27.07 0.52 0.70 3.14
C70 RG30 389.20 ± 31.6 0.58 ± 0.17 0.51 ± 0.13 0.32
C45RG30B25 417.9 ± 31.60 0.74 ± 0.20 0.65 ± 0.02 1.51
C40RG30B30 485.3 ± 31.6 1.20 ± 0.04 1.11 ± 0.16 1.47
C35RG30B35 595.8 ± 50.4 1.47 ± 0.43 1.36 ± 0.37 1.78
C45RG30SB25 462.7 ± 12.4 1.43 ± 0.36 1.32 ± 0.03 1.57
C40RG30SB30 408.3 ± 53.4 0.94 ± 0.29 0.85 ± 0.22 1.43
C35RG30SB35 303.1 ± 27.6 1.30 ± 0.33 1.08 ± 0.30 1.50
C: Castor oil cake; RG: Recovered/Crude Glycerol; B: Banana fiber; SB: Sugarcane bagasse Fiber
Table 2: Tensile properties of Castor oil cake-recovered glycerol and banana fiber /sugarcane bagasse green composites