Reinforcement (% wt.) Tensile strength (MPa) Flexural strength (MPa)
BN* BB** BN* BB**
0 26.9 ± 1.3 26.9 ± 1.3 25.4 ± 0.1 25.4 ± 0.1
10 26.3 ± 0.2 28.6 ± 0.3 30.9 ± 0.1 29.8 ± 0.0
15 23.8 ± 0.5 26.9 ± 0.3 31.3 ± 0.4 30.7 ± 0.2
20 24.8 ± 0.2 27.1 ± 1.1 35.1 ± 1.2 31.3± 0.2
BN (bagasse in nature); BB** (benzoylated bagasse).
Table 4: Mechanical results for tensile and flexural properties for PP composites reinforced with non-modified and benzoylated fibers.