S.NO. Sample ID Tensile strength (MPa) % Reduction in tensile strength Elongation at break (%) % Reduction in elongation
1 PP Virgin-MD 50.17 100 18.5 100
2 PP Virgin TD 48.25 100 125.1 100
3 PP-Fe MFA 1% D0 MD 48.46 96.59 16.3 88.11
4 PP-  Fe MFA 1% D0 TD 35.80 74.19 80.27 64.16
5 PP- Fe MFA 1% D1 MD Become Brittle
6 PP- Fe MFA 1% D1 TD Become Brittle
7 PP- Fe MFA 2% D0 MD 35.0 69.76 9.4 50.81
8 PP- Fe MFA 2% D0 TD 32.0 66.32 75.3 60.19
9 PP- Fe MFA 2% D1 MD Become Brittle
10 PP- Fe MFA 2% D1 TD Become Brittle
11 PP- Fe MFA 3% D0 MD 35.9 71.55 6.2 33.51
12 PP- Fe MFA 3% D0 TD 24.85 51.50 61.3 49.00
13 PP- Fe MFA 3% D1 MD Become Brittle
14 PP- Fe MFA 3% D1 TD Become Brittle

MD-Machine direction, TD-Transverse direction
D0= without UV Exposure, D1=One day UV Exposure
Table 1: Effect of MFA on mechanical properties of PP- Fe MFA before and after UV exposure .